Team:Imperial/Mechanical Testing
From 2014.igem.org
Line 52: | Line 52: | ||
<li>Created a size and quality optimised gif for visualisation of the experiment and written protocol for future iGEM teams to do the same. | <li>Created a size and quality optimised gif for visualisation of the experiment and written protocol for future iGEM teams to do the same. | ||
</li> | </li> | ||
- | + | ||
- | + | ||
Revision as of 02:23, 17 October 2014
Mechanical Testing
Overview
To check the feasibility of using our bacterial cellulose as a customisable ultrafiltration membrane, the mechanical properties were tested. For this to work, we checked the tensile strength of our filter, calculated the shear stress and estimated the processing method that produces membrane with the longest life-time. Our ultimate tensile stress calculated matched with literature values of bacterial cellulose within standard deviation, and the data analysis provided the insight to use non-blended cellulose rather than blended..
Key Achievements
- Introduced a new aspect to the manufacturing track in terms of quantitatively characterising the mechanical properties of our product, bacterial cellulose
- Quantified the tensile stress-strain properties of our bacterial cellulose.
- Established the feasibility of using bacterial cellulose as a customisable ultrafiltration membrane with water pressures of 75 bar within a conservative safety margin.
- Discovered that non-blended compared to blended bacterial cellulose was significantly more ductile, and would have longer life time as water filter, which informed the choice of cellulose for the final product.
- Tested and analysed 20 samples of bacterial cellulose test pieces.
- Created a size and quality optimised gif for visualisation of the experiment and written protocol for future iGEM teams to do the same.
Introduction
“How long would the bacterial cellulose water filter last? What will be the pressure we can apply on to it?” - Dr. Chipps (Principal Research Scientist at Thames Water)
The most accessible method of finding an answer to Dr. Chipps’ questions is to asses the quality of our material by pulling a test piece until it breaks, a tensile test. The quality of our bacterial cellulose will determine the water pressure that can be applied to it in a membrane bioreactor setting as the filter will be used in a flat orientation. Since the water pressure is the major limiting factor of the flow rates produced in such a setting, a key step to establishing the feasibility of our project is to perform a tensile test.
Tensile testing of bacterial cellulose is a common way of characterising and comparing its mechanical properties (Sherif 2006, Cheng 2009, Shezad 2010) and provides an indication of the orientation of the fibres in the bacterial cellulose pellicle. Therefore, we contacted Dr. Angelo Karunaratne of the Royal British Legion Centre of Blast Injury Studies at Imperial College, requesting access to test samples in an Instron 5866 materials testing machine (Instron Inc., Norwood, USA). Luckily Angelo was welcoming to the idea and allowed us to perform tensile stress-strain tests of our material. The aim was to calculate the young’s modulus, maximum stress applied and strain at failure.
Methods
Samples were prepared by oven drying at 60°C for 6 hours between VWR 413 filter paper, without pressure. Subsequently, samples were kept at room temperature (20°C) before testing. Cellulose was cut into 0.1 mm x 11 mm x 32 mm dumbbell shapes according to the recommendation from the ISO 527-3 guidelines for determination of tensile properties of plastics. Dumbbell shapes have the advantage of avoiding stress concentration at the clamps, and the dimensions chosen were sufficiently similar to existing literature dimensions, 0.16 mm×100 mm×150 mm to allow for comparison across studies (Sherif 2006). A digital vernier calliper was used to measure the thickness of each of the samples. 8 samples were used for the main cellulose fabric intended for water filtration, fewer were used for alternatively processed samples due to limited availability.
The test involves clamping test pieces into the Instron machine, moving the upper clamp upwards at a specific rate, ‘elongation time’, set to 20 mm/min to match that of existing literature (Sherif, 2006) and tracking the tensile force this introduces in the BC sample until the sample breaks, failure. Stress(σ) was calculated as the tensile force divided by the cross sectional area measured as width x thickness. Young’s modulus was calculated as stress/strain. Strain (ε) was calculated as ΔL/L0where ΔL is the elongation from the initial length L0.Samples were tested until visually confirming failure as shown in figure 3.
Two main sample types were tested. The BC pellicles intended for water filtration were immersed in a solution of Active Oxygen Fabric Stain Remover dissolved in distilled water. After 4 days, the pellicles were removed from the container, cut into squares of 5 cm by 5 cm, and allowed to dry between VWR 413 filter paper in an oven at 60°C for 3 hours. Then, the BC layered in filter paper was moved to room temperature, folded in Blue Roll, clamped between heatproof mats with mechanical clamps and left for 24 hours. This type of cellulose will be referred to as non-blended BC.
Alternative BC samples were treated in a 0.1 M NaOH solution in 80C for 3 hours, upon which it was dried off with blue roll and immersed in distilled water. After being in the distilled water solution for 12 hours, the BC was dried of with blue roll and blended in a Jamie Oliver food processor for 12 min at speed 2.
Results
The results of the mechanical tests of blended BC and non-blended BC are shown in table 1. The corresponding measurement data are shown in figure 3 and 4. As shown in table 1, the E, σand ε of non-blended BC was 1.52 MPa, 30 MPa and 35%, respectively. 10 samples were tested to check for variability in the cellulose samples produced as graphed in figure 5.
Sample processing | Ultimate tensile stress (MPa) | Yield stress (Mpa) | Young's modulus (Mpa) | Strain at break (%) |
---|---|---|---|---|
Non-blended bacterial cellulose | 29.9 ± 6.4 | 25.2 ± 7.2 | 1.5 ± 0.1 | 21 ± 3 |
Blended bacterial cellulose | 208 ± 80 | 155 ± 11 | 50.5 ± 1 | 4.1 ± 0.9 |